QC Issue ID
1
19
Drag to adjust the number of frozen columns
Select Batch
Describe Issue
Corrective Actions Taken
Follow Up Required
Status
Category
Resolution/Findings
21-001
Oh no, the kiln lost power halfway through curing and was off for 3 hours! Curing proceeded as normal after the outage. Will the malt color be different for this batch compared to typical spec?
n/a
Compare color with previous batches using hot steep method and Hartwick analysis.
Resolved
Kiln